Minimum Values |
Typical Values |
Typical composition after Sintering |
|||||||||||||||||
Code |
Tensile Properties |
Hardness |
Density |
C |
Cr |
Ni |
Mo |
Cu |
Nb |
Mn |
Si |
P |
Other |
Fe |
|||||
Uitimate Strength Rm |
Yield Strength Rp0.2 |
Elonga-tion A10 |
as sintered |
case hardened |
|||||||||||||||
Macro |
Micro |
Macro |
Micro |
||||||||||||||||
MPa |
MPa |
% |
HV10 |
HV10 |
HV10 |
HV10 |
g/cm³ |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
|
17-4PH |
950 |
660 |
3 |
320 |
7.6 |
≤0.07 |
15-17.5 |
3-5 |
3-5 |
0.15-0.45 |
≤1 |
≤1 |
Balance |
||||||
as sintered |
|||||||||||||||||||
17-4PH |
1100 |
950 |
5 |
370 |
7.6 |
≤0.07 |
15-17.5 |
3-5 |
3-5 |
0.15-0.45 |
≤1 |
≤1 |
Balance |
||||||
heat-treated |
|||||||||||||||||||
316L |
510 |
180 |
50 |
120 |
7.9 |
≥0.03 |
16-18 |
10-14 |
2-3 |
3-5 |
≤2 |
≤1 |
Balance |
||||||
310 N₂-sintered |
800 |
450 |
16 |
235 |
7.72 |
0.20-0.50 |
24-26 |
19-22 |
1.2-1.5 |
≤1.5 |
0.75-1.30 |
≤2.0 |
|||||||
HV1 |
|||||||||||||||||||
310 Ar-sintered |
600 |
250 |
40 |
160 |
7.65 |
0.20-0.50 |
24-26 |
19-22 |
1.2-1.5 |
≤1.5 |
0.75-1.30 |
≤12.0 |
Balance |
||||||
HV1 |
|||||||||||||||||||
420 heat-treated |
1600 |
1300 |
2 |
460 |
≥7.3 |
0.18-0.30 |
12.0-14.0 |
≤1.00 |
≤1.00 |
Balance |
|||||||||
430 |
350 |
200 |
30 |
150 |
100 |
≥7.6 |
≤0.08 |
15.5-17.5 |
≤1 |
≤1 |
Balance |
||||||||
430 |
Good corrosion resistance against water and steam |
400 |
750 |
≥7.60 |
0.90-1.25 |
16-18 |
≤0.60 |
≤0.75 |
2.5-3.5 |
≤1.0 |
≤1.0 |
≤0.040 |
S≤0.030 |
Balance |
Material |
Minimum Values |
Typical Values |
Typical composition after Sintering |
||||||||||||||
Code |
Tensile Properties |
Hardness |
Density |
C |
Cr |
Ni |
Mo |
Mn |
Si |
P |
S |
Fe |
|||||
Uitimate Strength Rm |
Yield Strength Rp0.2 |
Elonga-tion A10 |
as sintered |
case hardened |
|||||||||||||
Macro |
Micro |
Macro |
Micro |
||||||||||||||
MPa |
MPa |
% |
HV10 |
HV10 |
HV10 |
HV10 |
g/cm³ |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
|
1010 |
400 |
230 |
26 |
740 HV1 |
690 HV1 |
7.5 |
≤0.15 |
0.30-.066 |
≤0.4 |
≤0.045 |
≤0.045 |
Balance |
|||||
4140 as sintered |
650 |
400 |
3 |
230 |
130 |
7.4 |
0.32-0.42 |
0.90-1.20 |
0.15-0.30 |
Balance |
|||||||
4140 heat-treated |
1450 |
1250 |
2 |
450 |
7.4 |
0.32-0.42 |
0.90-1.20 |
0.15-0.30 |
Balance |
||||||||
4605 as sintered |
600 |
400 |
5 |
150 |
7.55 |
0.4-0.6 |
1.5-2.5 |
0.2-0.5 |
Balance |
||||||||
4605 heat-treated |
1300 |
1100 |
5 |
390 |
7.55 |
0.4-0.6 |
1.5-2.5 |
0.2-0.5 |
≤1.0 |
Balance |
|||||||
1900 |
1500 |
2 |
600 |
||||||||||||||
FN02-2% Nickel Steel |
260 |
150 |
25 |
110 |
90 |
600 |
7.5 |
≤0.1 |
1.9-2.2 |
≤1.0 |
Balance |
||||||
FN08-8% Nickel Steel |
380 |
210 |
15 |
140 |
90 |
600 |
7.5 |
≤0.1 |
7.5-8.5 |
Balance |
Material Code |
Minimum Values |
Typical Values |
Typical composition after Sintering |
||||||||||||||
Density |
Permeability μmах |
Magnetic Properties |
Tensile Properties |
C |
Cr |
Ni |
Mn |
Si |
Fe |
||||||||
Maximum Polarization Js (4kA/m) |
Coercivity Hc |
Residual Induction Br |
Ultimate Strength Rm |
Yield Strength RP0.2 |
Elonga-tion A10 |
Hardness |
|||||||||||
g/cm³ |
T |
A/m |
T |
MPa |
MPa |
% |
HV1 |
wt% |
wt% |
wt% |
wt% |
wt% |
wt% |
||||
430 |
≥7.6 |
3311(@p=6.68 cm3) |
1.335 (@p=7.68 cm3) |
73 (@ p= 7.68 cm3) |
0.639 (@ p= 7.68 cm3) |
≥350 |
≥200 |
30 |
100-150 HV10 |
≤0.08 |
15.5-17.5 |
≤1 |
≤1 |
Balance |
|||
FeSi3 |
≥7.5 |
5215(@ p= 7.66 cm3) |
1.573 (@ p= 7.66 cm3) |
73 (@ p= 7.68 cm3) |
1.154 (@ p= 7.66 cm3) |
≥500 |
≥300 |
20 |
120-160 |
≤0.10 |
2.5-3.0 |
Balance |
|||||
FN50-50% 20Nickel Steel |
≥7.6 |
27270 (@ p= 7.8 cm3) |
1.356 (@ p = 7.8 cm3) |
10 (@ p= 7.8 cm3) |
0.8 (@ p= 7.8 cm3) |
≥400 |
≥150 |
20 |
100-140 |
≤0.10 |
49.5-50.5 |
Balance |
|||||
Pure%20 lron |
≥7.8 |
14236(@p=7.83 cm3) |
1.635 (@p=7.83 cm3) |
29 (@ p= 7.83 cm3) |
1.244 (@ p= 7.83 cm3) |
≥230 |
≥110 |
40 |
50-60 HV10 |
≤0.1 |
Balance |